When a tungsten carbide seal ring develops a chip at its inner diameter (ID) or outer diameter (OD), the immediate reaction is often to blame carbide brittleness or material quality.

Sometimes the grade really is part of the problem. But in many failed seals, the chip location tells us something more useful: where mechanical, thermal, assembly, or contact stress became concentrated.

I pay particular attention to whether the damage starts at the ID, the OD, the lapped face edge, a drive notch, or a mounting surface. A small chip at one of these locations is not random. It is often the first visible evidence of how the ring is being loaded inside the seal.

Why Carbide Seal Ring Edges Are More Vulnerable Than the Main Face

Cemented carbide is designed to combine very high hardness with usable toughness. The WC grains provide wear resistance, while the metallic binder helps the material resist fracture.

But an edge is mechanically different from the middle of a thick, supported section.

At the ID or OD, the carbide has less surrounding material to distribute load. A sharp corner can therefore concentrate stress from:

● Impact during handling

● Pressing into a holder

● Uneven face loading

● Drive torque

● Shaft movement

● Thermal expansion

Once a microcrack begins at the edge, repeated loading can extend it into the ring. This is why edge geometry, chamfers, radii, and support deserve as much attention as hardness.

Why Tungsten Carbide Seal Rings Chip at ID or OD.png

1. Why Tungsten Carbide Seal Rings Chip at the Inner Diameter

Inner-diameter chipping should make you inspect everything physically or mechanically connected to the bore.

Shaft or Sleeve Contact

If the ID provides clearance around a shaft or sleeve, abnormal shaft movement can bring rotating metal dangerously close to the carbide edge.

Causes may include:

● Excessive shaft runout

● Bearing wear

● Shaft deflection

● Incorrect seal centering

● Assembly eccentricity

A narrow chip or polished mark at one ID location is often more consistent with local contact than with a uniformly weak carbide grade.

Too-Small ID Chamfer

A perfectly sharp carbide edge may look precise on a drawing, but it is also more vulnerable during assembly. If the ring passes over a shaft shoulder, sleeve step, key feature, or installation tool, a controlled edge break can reduce accidental impact.

The chamfer should still be designed so that it does not reduce the required sealing width or interfere with another component.

Secondary-Seal or Drive Loading Near the ID

Some seal designs transfer force close to the ring bore through O-rings, drive elements, retainers, or supporting hardware. If the load is concentrated rather than distributed, the ID region may experience local tensile or bending stress.

When the same ID sector chips repeatedly, I would inspect the orientation of every drive pin, notch, spring, or holder feature before changing the carbide grade.

2. Why Tungsten Carbide Seal Rings Chip at the Outer Diameter

OD chipping more often directs my attention toward the holder, press fit, drive mechanism, installation method, or exposed outside edge.

Excessive Interference Fit

A carbide ring mounted in a steel holder is not simply an OD dimension inserted into an ID dimension. It is a mechanical fit involving materials with different stiffness and thermal expansion behavior.

Too much interference can place excessive stress into the carbide. Uneven holder geometry can make that stress even worse.

This is particularly important for thin-wall custom tungsten carbide seal rings, where the same dimensional interference represents a more severe condition than it would in a thick section.

Installation Impact

Carbide rings should not be driven into position by direct metal hammering or by applying point loads to an edge.

A ring may survive assembly and show no immediately visible crack, then chip during startup when pressure, temperature, and rotation add another load cycle.

Drive Pin or Anti-Rotation Contact

Drive features are common locations for localized stress. AESSEAL specifically notes that optimized drive lugs and spring arrangements are used to reduce face damage and prevent springs from directly damaging or chipping hard seal faces.

If OD chipping aligns with a drive pin, lug, notch, or retaining feature, that correlation should be investigated.

3. Thermal Distortion Can Load Either the ID or OD Edge

Mechanical seal faces generate and absorb heat during operation. If lubrication deteriorates, face friction rises and temperature gradients become more severe.

The carbide ring, metal holder, shaft, and surrounding seal hardware may expand differently. As a result, a fit or loading condition that is acceptable when cold can change at operating temperature.

Rapid temperature change can add another risk. A locally overheated face followed by sudden cold flush, product change, or shutdown cooling can create thermal stress around existing edge defects.

4. Dry Running and Poor Lubrication Can Lead to Edge Chipping

A conventional contacting mechanical seal depends on a very thin lubricating film between its faces. Poor lubrication increases friction and heat generation.

High spots may then carry more load, while thermal distortion changes the contact pattern. Instead of the complete face sharing load evenly, contact may move toward the ID or OD.

This matters because a chip can be the final event rather than the first failure mechanism.

The real sequence may be:

poor lubrication → heat → face distortion → edge loading → microcrack → chip.

Our article on seal-face flatness and lapping quality explains why loss of flatness changes contact distribution and sealing behavior.

5. Abrasive Solids Can Attack the Seal Face Edge

In slurry, wastewater, mining, and dirty process service, hard particles can enter the seal interface.

An isolated particle trapped near the ID or OD can create a local indentation or chip, particularly if it is larger than the normal lubricating-film thickness.

Repeated solids circulation may also erode the face boundary until an edge becomes unsupported.

This is why tungsten carbide seal rings for abrasive mechanical seals should be selected together with an appropriate flushing or barrier strategy.

A harder face does not make abrasive particles disappear.

6. The Carbide Grade May Be Too Brittle for the Geometry

Grade selection still matters.

Cemented carbide properties depend strongly on binder content and WC grain size. A grade optimized for maximum hardness and abrasion resistance may not be the best choice for a thin ring exposed to vibration, impact, aggressive drive loading, or repeated thermal cycles.

Higher toughness can sometimes be more valuable than a small increase in hardness.

That does not mean increasing binder content blindly. The seal still needs wear resistance, corrosion compatibility, dimensional stability, and suitable face performance.

My preferred sequence is:

identify the fracture mechanism first → then decide whether grade toughness is actually inadequate.

7. Grinding and Lapping Can Leave a Vulnerable Edge

Carbide seal rings are normally ground and the working face may be precision lapped. These processes must finish the component without leaving deep grinding damage or microchipping at the perimeter.

A lapped face can appear excellent while the ID or OD edge contains small defects from an earlier grinding operation.

Final inspection should therefore include more than flatness and Ra.

Inspect:

● ID and OD edge continuity

● Chamfer consistency

● Drive notches and slots

● Grinding marks

● Microchips

● Surface cracks

For repeat orders of precision tungsten carbide seal rings, critical edge conditions should be included on the drawing rather than left to a vague note such as “break all sharp edges.”

tungsten carbide mechanical seal rings high wear resistance carbide seals .png

When customers send us a chipped seal ring, I do not begin by recommending a harder or tougher grade.

I first look at where the chip begins.

ID damage makes me think about shaft clearance, centering, and bore-side loading. OD damage makes me look harder at the holder, interference, drive mechanism, and installation. Chipping around both edges makes manufacturing, handling, and thermal history more important.

Only after those possibilities are reviewed does material grade become the main question.

Langsun Carbide manufactures tungsten carbide seal rings for mechanical seals in application-specific dimensions, WC-Co or WC-Ni binder systems, custom edge geometry, precision-ground dimensions, and lapped sealing surfaces according to customer drawings.

A chip is rarely just missing material. It is evidence showing where the seal system concentrated stress.

FAQ

Why does a tungsten carbide seal ring chip at the inner diameter?

Common causes include shaft or sleeve contact, insufficient ID clearance, poor centering, sharp edge geometry, assembly impact, or localized loading from nearby seal hardware.

Why does the outer diameter chip after press fitting?

Excessive interference, an out-of-round holder, uneven pressing, insufficient chamfer, or point loading can create damaging stress in the OD region.

Does chipping mean the carbide grade is too brittle?

Not necessarily. Grade toughness may contribute, but chipping can also result from installation, alignment, thermal distortion, dry running, abrasive contamination, or concentrated mechanical loading.

Author | Allen

Allen is the International Marketing Director at NINGBO LANGSUN TUNGSTEN CARBIDE CO., LTD. With more than five years of experience in industrial wear parts and Tungsten Carbide Applications, he works with mechanical-seal companies, pump manufacturers, OEMs, and procurement teams on material selection, drawing review, failure analysis, manufacturing feasibility, and quality-control requirements.

Facebook: Allen on Facebook
LinkedIn: Allen on LinkedIn

References

1. CERATIZIT, Cemented Carbide. Technical overview of WC hard phase, metallic binder, binder content, grain size, toughness, hardness, and other application properties. 

2. Jewell, P. et al., “Rate and Microstructure Influence on the Fracture Behavior of Cemented Carbides WC-Co and WC-Ni,” International Journal of Fracture, 2017. 

3. AESSEAL, “SMSS Single Cartridge Seal.” Technical design information describing optimized seal-face drive and loading intended to reduce startup/shutdown damage and prevent direct spring-induced face chipping. 

4. John Crane, Type 2609HTL/3609HTL Technical Specification. Describes mating-ring designs that control radial and axial force and reduce thermal-growth-induced face distortion. 